Mechanical Properties | ||||
---|---|---|---|---|
BERYLCO ALLOY 14 (UNS 17510) | ||||
Temper | A (TB00) | H (TD04) | AT (TF00) | HT (TH04) |
Tensile Strength ksi | 35-55 | 65-80 | 100-130 | 115-140 |
Tensile Strength MPa | 240-380 | 450-550 | 690-895 | 793-960 |
0.2% Yield Strength ksi min. |
25 | 55 | 80 | 110 |
0.2% Yield Strength MPa min. |
170 | 380 | 550 | 760 |
Elongation in 4D% min. | 30 | 10 | 10 | 10 |
Hardness Rockwell | B 50 max | B 60-80 | B 92-100 | B 95-102 |
Electrical Conductivity %IACS min. |
20 | 20 | 45 | 48 |
Typical Age Hardening | — | — | 3 hrs. @840-900°F | 2 hrs. @840-900°F |
Typical Physical Properties | ||||
Density lbs./in3 @ 68°F | .317 | |||
Coefficient of Thermal expansion 68°F to 390°F |
10.0 x 10-6 | |||
Thermal Conductivity BTU/(ft. x hr. x °F) @ 68°F |
145 | |||
Electrical Conductivity %IACS @ 68°F |
48 | |||
Thermal Capacity (specific heat) BTU/(lb. x °F) @ 68°F |
0.1 | |||
Modulus of elasticity psi | 19.2 x 106 | |||
Modulus of rigidity (Torsion Modulus) psi |
7.5 X 106 | |||
Magnetic permeability | ||||
Machinability | 40 |