Alloy 17510 Properties
Mechanical Properties BERYLCO ALLOY 14 (UNS C17510) |
||||
---|---|---|---|---|
Temper | A (TB00) | H (TD04) | AT (TF00) | HT (TH04) |
Tensile Strength ksi | 35-55 | 65-80 | 100-130 | 115-140 |
Tensile Strength MPa | 240-380 | 450-550 | 690-895 | 793-960 |
Elongation in 4D% min. | 30 | 10 | 10 | 10 |
Hardness Rockwell | B 50 max | B 60-80 | B 92-100 | B 95-102 |
Electrical Conductivity %IACS min. | 20 | 20 | 45 | 48 |
Typical Age Hardening | — | — | 3 hrs. @840-900°F | 2 hrs. @840-900°F |
Specifications
ASTM |
B441, B534 |
Federal |
|
AMS |
|
RWMA |
Class 3 |
CDA |
C17510 |
DIN |
1777 and 1791 |
Outstanding Characteristics
- Good strength
- Good fatigue strength
- High conductivity